Epoxy casting looks simple—mix two liquids and pour—but dependable results come from controlling four variables: ratio, mixing, depth and temperature. This beginner-friendly guide explains a repeatable process for small home-decor pieces, silicone molds, adult craft kits and workshops.
Start with the product instructions
Every epoxy system has its own mixing ratio, working time, maximum pour depth and curing schedule. Treat the manufacturer’s label and safety data as the primary source. Do not borrow a ratio from another resin, and never add extra hardener to speed curing; that usually creates a soft, sticky or brittle result.
Work in a ventilated area. Protect the work surface, wear the personal protective equipment specified by the manufacturer, keep food and drinks away, and prepare all tools before opening the containers.
Measure the mold before mixing
For a new silicone mold, estimate the required volume before handling resin. One practical method is to fill the empty mold with water, pour the water into a measuring cup and record the volume. Then dry the mold completely—water must not enter the epoxy.
This step reduces waste and is especially useful when planning a workshop or assembling creative kits for adults. Add only the small margin recommended for transfer loss rather than mixing a large excess.
Use separate cups, then combine
For a two-part system, label three clean cups: A, B and A+B. Measure each component according to the stated ratio, using weight or volume exactly as the product specifies. Pour both components into the third cup.
Mix slowly and thoroughly for the required time. Scrape the sides, bottom and corners of the cup so no unmixed material remains. Incomplete mixing is one of the most common reasons a casting fails to cure.
Some makers use a second clean-cup transfer: after the first mix, pour into a fresh cup and mix again. This can reduce the chance that an unmixed film from the original cup reaches the mold, provided the product’s working time allows it.
Understand depth and curing
Two molds can hold the same volume and still cure differently. A deep heart and a shallow square may each contain 90 ml, but the deeper casting can warm and harden sooner because epoxy curing is exothermic. Shape and height matter, not only total quantity.
Never exceed the resin’s permitted pour depth. Thick pours can overheat, discolor, crack or damage a mold. If a piece is too deep for one pour, use layers according to the manufacturer’s recoating window.
Color without losing control
Finish the complete A+B mix before adding decorative effects. Then divide the mixed resin among smaller cups and add only pigments, mica, inks or metallic leaf confirmed as compatible with epoxy.
For a galaxy-style effect, pour narrow bands of several colors and draw a clean stick through the bands in the direction of the pour. Avoid overworking; too much movement can turn distinct colors muddy.
Reduce bubbles deliberately
Stir slowly rather than whipping air into the mixture. Pour in a thin stream and inspect mold corners. Gentle warmth can lower viscosity, but heat also shortens working time and increases the exothermic reaction. Use only a warming or bubble-removal method allowed by the specific resin manufacturer, and never improvise with open flame around flammable materials.
Flowers and inclusions
Use fully dried flowers. Moist plant material can create cloudiness, bubbles or poor curing. For better placement, coat each flower with a little mixed epoxy before setting it into a thin first layer. Allow that layer to reach the stage required by the product, then add the next layer. Pre-coating helps release trapped air and reduces floating.
Troubleshooting
Sticky or soft areas usually point to the wrong ratio, incomplete mixing, low temperature or disturbing the piece too early. Clusters of bubbles often come from fast stirring, porous inclusions or trapped air in fine mold details. Uneven color can result from incompatible pigment or insufficient mixing after the resin has been divided.
Record the product, ratio, room temperature, mold depth, pigment amount and timing for every test. A simple log turns mistakes into a repeatable process.
The original GRAYISH tutorial, including videos on mixing, drying, color effects and flowers, is available on the GRAYISH website.